A hotend with a fan duct blowing air onto a freshly printed layer, with a fan speed graph rising across layers

Once melted plastic leaves the nozzle, it has to cool and harden before the next layer goes on top. The part cooling fan controls how fast that happens. Too little cooling and overhangs droop, corners round off and small parts melt into blobs. Too much and layers bond poorly, parts crack along the layer lines and the first layers curl off the bed.

Slicers give you a handful of cooling settings. This guide explains what each one does, with the setting names used by OrcaSlicer and Bambu Studio, which are close to the names in PrusaSlicer and Cura.

What the fan is for

The part cooling fan blows air through a duct onto the plastic just after it leaves the nozzle. It is separate from the fan that cools the heat sink above the hotend, which stays on all the time.

Cooling matters most in three places:

  • Overhangs and bridges, where plastic has nothing below it and must stiffen quickly to hold its shape.
  • Small parts and thin tips, where each layer is so short that the previous layer has not had time to cool.
  • Fine details and sharp corners, which stay crisp when each layer hardens before the next arrives.

Cooling matters less, or even works against you, for strength. A hotter layer bonds better to the one below it, so a part that must be strong is usually printed with less cooling.

The settings, one by one

Close the fan for the first layers

OrcaSlicer's documentation describes a setting called close fan the first N layers. It sets how many of the first layers print with the part fan off. This helps the first layers stick to the bed and reduces early warping. The auxiliary fan, if the printer has one, is also off for these layers.

Most default profiles turn the fan off for the first layer or a few layers. Leave it that way unless a first layer problem points to cooling. If you see the bottom layers lifting at the corners, make sure this value is not set to zero. The warping guide explains why bed-level cooling lifts corners.

First layer fan speed

OrcaSlicer also has a setting for a fixed fan speed on the first layer. It overrides the other cooling settings for that layer and can help cool the toolhead ducts on a hot bed without cooling the plastic fully. Normal cooling resumes from the second layer. According to the documentation, it only works when the close-fan value is zero, and setting it to minus one disables it.

Full fan speed at layer

Instead of jumping from off to full speed, the slicer can ramp the fan up gradually. The OrcaSlicer documentation explains that this setting raises the fan linearly from 0% on the first layer after the close-fan period to the maximum part-cooling speed at the layer you choose. If you set it to zero, the ramp is disabled.

A gentle ramp is a good choice for filaments that dislike sudden cooling, because it avoids a hard change right where the first layers end.

Minimum and maximum fan speed

These two numbers set the range of the fan. The slicer chooses a speed between them according to how long each layer takes to print. Layers that print quickly, such as the tip of a small part, get more cooling. Layers that take longer, such as a large flat area, get less.

Layer time thresholds and slowdown

The slicer estimates how long each layer takes. If a layer is shorter than the minimum layer time, the fan speeds up and the printer can slow down to give the plastic time to cool. This is why a tiny part prints slower than a big one even when you set the same speed.

If a small part still sags at its tip after the fan is already at maximum, the fix is usually to give each layer more time, either by slowing it down or by printing two copies at once so the nozzle spends time on the other part.

Overhang and bridge cooling

OrcaSlicer's documentation describes a setting that forces extra cooling for overhangs and bridges. There is an activation threshold, which is how much of a line's width has to be unsupported before the fan boosts, with options of 0%, 10%, 25%, 50%, 75% and 95%. At 0% the fan runs at that speed for all outer walls. The overhang fan speed then applies to bridges and overhang walls above the threshold. It is never set below the minimum fan speed.

PrusaSlicer has a similar feature called dynamic fan speeds. According to a clarification quoted in the comments of Prusa's knowledge base article, the dynamic values override the maximum in the fan settings. For example, with a maximum of 50% and a dynamic setting of 100%, the fan runs at full speed when the overhang conditions are met. The lower the overlap with the layer below, the higher the fan speed should be.

For problems at overhangs and bridges, see overhang problems and bridging settings.

Auxiliary fan

Some printers have a second part cooling fan. OrcaSlicer's setting for it controls its speed and keeps it off during the first layers set by the close-fan option. If your printer has one, it needs no special treatment beyond leaving the profile's value in place.

Guidance by material

Use the slicer's built-in profile for your printer and filament as the starting point. These notes explain why the profiles differ.

Material Cooling Why
PLA High Cools and hardens fast, holds sharp corners and bridges with strong airflow
PETG Medium Needs enough cooling for overhangs, but too much weakens layer bonding and can cause cracks
ABS and ASA Low or off Shrinks as it cools, so heavy airflow causes warping and splitting between layers
TPU Low to medium Prints slowly, so extra cooling is usually less important

If your filament manufacturer prints a recommended fan range on the spool or the product page, follow that first. For more on each material, see the PETG printing guide and the ABS printing guide.

Signs of too little cooling

  • Overhangs droop or curl upward at the edges.
  • Corners on small parts look rounded, and the tips of thin features melt together.
  • Bridges sag in the middle.
  • The surface looks shiny and slightly melted on small layers.

Signs of too much cooling

  • Layers separate or crack along the layer lines, especially on tall parts. See layer separation.
  • The first layers curl up at the corners.
  • Under-extrusion on the first few layers because the nozzle cools down. Watch the nozzle temperature graph on your printer if it has one.
  • Parts that are weak even though they look good.

A simple way to tune it

  1. Print an overhang test or a small model with tall thin features, using the slicer's default profile for your filament.
  2. If overhangs droop, raise the overhang fan speed or enable the extra cooling for overhangs and bridges.
  3. If layers split, lower the maximum fan speed by 10–20 percentage points and print again.
  4. If small parts melt, raise the minimum layer time so the printer slows down on short layers.
  5. Change only one setting between prints and write it on the test part.

Remember that cooling interacts with temperature. A slightly lower nozzle temperature cools the plastic faster, which can help overhangs without a higher fan speed. The temperature tower guide shows how to find the best temperature for a spool.

Frequently asked questions

Should I turn the part cooling fan off for the first layer?

Yes, for most materials. Cooling the first layers makes it harder for plastic to stick, and corners can lift. Profiles usually turn the fan off for the first layer or a few layers and ramp up afterwards.

Does the part cooling fan affect strength?

Yes. More cooling makes a layer harden before the next one bonds well, which can weaken the part. For strong parts, use less cooling, within what the material allows.

Why does my printer slow down on small parts?

The slicer enforces a minimum layer time. When a layer would take less time than that, it slows the print so the plastic can cool. Printing several copies together or lowering the minimum layer time changes this.

Can I print ABS with the fan on?

Heavy cooling causes warping and layer splitting in ABS, so most profiles keep the fan low or off. A small amount of cooling for overhangs may be fine, but follow your printer's ABS profile first.

What is the difference between the part cooling fan and the hotend fan?

The hotend fan keeps the heat sink above the nozzle cool so filament does not soften too early. It runs all the time. The part cooling fan cools the printed plastic and is controlled by your slicer settings.